Equivalent alloy:
GH4080A(China), UNS N07080 Nimonic80A (US)
The chemical composition of the Nimonic80A:
Alloy |
% |
NI |
CR |
FE |
MN |
SI |
P |
S |
Al |
TI |
C |
CO |
B |
ZR |
CU |
Nimonic80A |
The minimum |
Margin |
18 |
|
|
|
|
|
1.0 |
1.8 |
|
|
|
|
|
The maxmum |
amount |
21 |
3.0 |
1.0 |
1.0 |
0.02 |
0.015 |
1.8 |
2.7 |
0.1 |
2.0 |
0.008 |
0.15 |
0.2 |
The Physical properties of the Nimonic80A:
The density |
8.19 g/cm3 |
Melting point |
1320-1365℃ |
Nimonic80Aalloy's mechanical properties at room temperature, the minimum value:
Alloy |
Tensile strength |
The yield strength |
elongation |
Nimonic80A |
930 |
620 |
20 |
The alloy has the following features:
Main features: using temperature 700-800℃, in 650-850℃with good creep resistance and oxidation resistance. Precipitation hardening alloys, high temperature (815 ° C) for excellent properties.
Cold and hot deformation performance is good, used in the manufacture of engine rotor vane and guide vane bearings, bolts, lock plate in blade and other parts.
The above data is for your reference, should you have any special requirements, please contact us!